Mortar types N, S, M and O: laboratory minimums from 350 to 2,500 psi

Plain-English mortar guidance for bricklayers and site work

Mortar Smash › Trade guides › Mortar types N, S, M and O

By the Mortar Smash editorial team. Published 5 November 2026. Sources re-read 21 November 2026.

Short answer

Type M, S, N and O are the four mortar types in ASTM C270. BIA Technical Note 8 (March 2020), Table 2, sets the minimum average compressive strength at 28 days for laboratory-prepared mortar at 2,500 psi for M, 1,800 psi for S, 750 psi for N and 350 psi for O. Those numbers are a laboratory floor. A cube taken on the mortar board is not the test that passes or fails the type. For ordinary work, including most veneer, the same note says to use Type N, and to pick the type from Technical Note 8B. The project specification and the local code still govern the wall in front of you.

Fresh grey mortar in a wheelbarrow with a brick trowel beside a stack of red clay bricks
Illustrative AI-generated photo of site-mixed mortar and bricks. Image policy.

The laboratory floors, from Table 2

Table 2 of Technical Note 8 is headed as property-specification requirements, and note a says the figures are for laboratory-prepared mortar only. The minimum average compressive strength at 28 days is the same for cement-lime, mortar cement and masonry cement:

Type28-day lab minimumWater retention, minimumAir content, maximum, cement-lime
M2,500 psi (17.2 MPa)75%12%
S1,800 psi (12.4 MPa)75%12%
N750 psi (5.2 MPa)75%14% (12% if the cement-lime mortar contains structural reinforcement)
O350 psi (2.4 MPa)75%14% (12% if the cement-lime mortar contains structural reinforcement)

Mortar cement and masonry cement have higher air-content ceilings in the same table: 18% for M and S, and 20% for N and O, cut to 18% when structural reinforcement is in the mortar. Non-air-entrained portland cement-lime mortar is generally under 8% air, which is note b. These ceilings are limits, not a target to chase with an extra air-entraining agent. The note's summary says not to combine two air-entraining agents.

The psi column used to be easy to misread as a typical strength you should see in a bucket sample. Table 2 does not say that. It says "minimum" and "laboratory-prepared mortar only."

Why a site cube cannot pass the type

Technical Note 8 says properties of field-mixed mortar cannot be compared with the property specification. Laboratory mortar and field mortar use different amounts of water, different mixers and different curing. Field mortar is generally wetter, because the brick will pull water out of the joint, and it has a lower compressive strength than the laboratory mortar of the same type. Field sampling, where a specification asks for it, tracks consistency from the start of the job to the end. It is not the compliance test. Further detail is in Technical Note 8B, which this note points to and which we have not re-read as a separate PDF for this page.

The ASTM C270-25 store page, checked 21 November 2026, says the same thing in the abstract: the specification does not determine mortar strengths through field testing; compressive strength from field-tested mortar does not represent the laboratory strength or the mortar in the wall; physical properties of field-sampled mortar shall not be used to determine compliance and are not acceptance criteria. Compliance is checked by confirming that the specified materials meet their own requirements and go into the mixer in the proper proportions. We have not read the paywalled C270-25 tables. The psi figures and the volume bands on this page are the ones printed in Technical Note 8 (March 2020), which cites the 2019 Annual Book of ASTM Standards. If the edition named in the project specification differs, follow that edition.

Proportion is the default. Property is the lab route.

ASTM C270, as Technical Note 8 summarises it, allows two ways to specify a type. Proportion specifications mix materials to the volumes in Table 1, and they need no laboratory testing before or during construction. Property specifications require compressive strength, water retention and air content tests on laboratory mortar, mixed with a controlled amount of water, before construction. The quantities from that laboratory mix are then used in the field, with the mason choosing the water.

If the specification names neither route, the proportion specification governs. The exception in the note is a preblended dry mortar that complies with ASTM C1714: for that mix, the property specification is the default. A mortar batched to the proportion specification is not compared with a mortar of the same type batched to the property specification. The note, citing Melander and Conway (ASTM STP 1180, 1993), says the proportion mix will have a higher laboratory compressive strength than the property mix of the same type and the same cementitious materials. Bagged mixes are covered in preblended vs site-mixed mortar.

Cement-lime volumes in Table 1

For cement-lime mortar, Table 1 gives one part cement (ASTM C150, C595 or C1157) and a band of hydrated lime or lime putty. Sand is measured damp and loose, at not less than 2½ and not more than 3 times the sum of the cementitious volumes. That sand band belongs to the proportion table. The property table uses a different aggregate band, 2¼ to 3½ times, and that band is for the laboratory mix. A site batch following the proportion specification uses 2½ to 3.

TypeCementHydrated lime or lime puttySand at 1 part lime, or at the stated lime
M1¼Cementitious volume is 1¼. Sand is 3⅛ to 3¾.
S1over ¼ to ½At ½ lime, cementitious volume is 1½. Sand is 3¾ to 4½.
N1over ½ to 1¼At 1 lime, cementitious volume is 2. Sand is 5 to 6.
O1over 1¼ to 2½At 2 lime, cementitious volume is 3. Sand is 7½ to 9.

The sand column is the Table 1 multiplier applied to one lime figure inside each band. It is arithmetic on the printed ranges, not a separate recipe. Mortar cement and masonry cement are different rows: the note says to use them alone with sand, without added lime, to make type M, S, N or O. Type N mortar cement or masonry cement may be combined with portland cement to make type M or type S. Gauging a board from these bands is in how to mix mortar. Once the type is chosen, quantities of cement and sand for a wall are in the mortar calculator.

Type N for normal use, and where the choice actually lives

The opening summary of Technical Note 8 says to use Type N for normal use, including most veneer applications, and to select the mortar type using the recommendations of Technical Note 8B. Later, under recommended uses, the note says no single type is best for all brick units or applications, and it points to 8B again. Compressive strength, the note says, is not the primary consideration for brick mortar, especially veneer. Bond strength, workability and water retention should get the main attention when the mortar is chosen.

A job-by-job table, including walls at or below grade, is on which mortar for brickwork, cited there to the Acme Brick selection guide. Historic and soft brick, where a low-strength joint is the point, is in lime vs cement mortar and how to repoint brick. None of those pages, and not this one, is a structural design. Check the specification and the code that apply to the wall.

Mortar type FAQ

What are the laboratory strength minimums for mortar types M, S, N and O?

BIA Technical Note 8 (March 2020), Table 2, lists minimum average compressive strength at 28 days for laboratory-prepared mortar: Type M 2,500 psi (17.2 MPa), Type S 1,800 psi (12.4 MPa), Type N 750 psi (5.2 MPa) and Type O 350 psi (2.4 MPa). The same four figures apply to cement-lime, mortar cement and masonry cement. They are laboratory minimums, not a field-cube result.

Can a mortar cube taken on site prove ASTM C270 compliance?

No. The ASTM C270-25 store abstract says this specification does not determine mortar strength through field testing, and that physical properties of field-sampled mortar shall not be used to determine compliance. BIA Technical Note 8 says field mortar is generally wetter and weaker than laboratory mortar, and that field sampling tracks consistency. It is not the property-specification test.

Which mortar type does BIA name for ordinary veneer?

The summary of BIA Technical Note 8 (March 2020) says to use Type N mortar for normal use, including most veneer applications, and to select the type using Technical Note 8B. The same note says no single type is best for every brick and every job. The project specification and the local code still govern.

How much lime is in cement-lime Type N?

BIA Technical Note 8, Table 1, sets cement-lime Type N at 1 part cement to over ½ and up to 1¼ parts hydrated lime or lime putty, by volume. Sand, measured damp and loose, is 2½ to 3 times the combined volume of those cementitious materials. At 1 part lime, that sand band is 5 to 6 parts.

Are the letters M, S, N and O a UK classification?

They are the four types in ASTM C270, which is the US specification BIA Technical Note 8 is written around. A UK job follows the specification and the code for that job. Do not copy a US letter onto a UK drawing without checking those documents.

Sources

Re-read 21 November 2026. The sand volumes in the worked rows are the Table 1 multiplier (2½ to 3) applied to one lime figure inside each printed band. Codes and project specifications differ by country and job; where they conflict with this page, follow them. This is general information, not engineering advice.